355 N | 355EM / EMZ | S355G2+N | S355G3+N | S355G7+N S355G8+N S355G9+N S355G10+N |
API 2H-50 | e. g. E 36 / EH 36 |
Thick. [mm] |
Tensile strength Rm [MPa] |
|||||
≤25 | 460 – 620 | 470 – 630 | 470 – 630 | 470 – 630 | 483 – 620 | 90 – 620 |
> 25 ≤40 | " | " | " | " | " | " |
> 40 ≤100 | '' | - | '' | '' | '' | '' |
> 100 ≤150 | '' | - | - | '' | '' | '' |
Thick. [mm] |
Yield Strength ReH [MPa] |
|||||
≤16 | ≥355 | ≥355 | ≥355 | ≥355 | ≥355*) | ≥355 |
> 16 ≤20 | '' | ≥345 | ≥345 | '' | '' | '' |
> 20 ≤25 | '' | '' | '' | '' | '' | '' |
> 25 ≤40 | ≥345 | - | '' | ≥345 | '' | '' |
> 40 ≤63 | ≥340 | - | - | ≥335 | '' | '' |
> 63 ≤80 | ≥325 | - | - | ≥325 | ≥325*) | '' |
> 80 ≤100 | ≥325 | - | - | '' | '' | '' |
> 100 ≤120 | ≥315 | - | - | '' | '' | '' |
> 120 ≤150 | ≥305 | - | - | ≥320 | '' | '' |
*)Rp0.2
|
355 N | 355EM / EMZ | S355G2+N | S355G3+N | S355G7+N S355G8+N S355G9+N S355G10+N |
API 2H-50 | e. g. E 36 / EH 36 |
Minimum Impact Energy Av [Joule] - transverse (average/single) - at a test temperature of | ||||||
-40 oC | -40 oC | -40 oC | -40 oC | -40 oC | -40 oC | |
Surface All thickness < 40 mm < 50 mm |
50 / 35 - - |
50 / 35 - - |
50 / 35 - - |
50 / 35 - - |
- 41/34 - |
- - 24/17 |
Quarter thick. >40 > 50 < 70 > 70 < 150 |
- - - |
_ _ _ |
- - - |
- |
41/34 - - |
- 27 /19 34 / 24 |
Mid-thickness All thicknesses > 40 mm |
- 50 / 35 |
- - |
- - |
- 50 / 35 |
- - |
- - |